Controlled dewetting and phase transition hysteresis of VO2 nanostructures
Listen
Radio episode about this paper
Transcript
Introduction to the show: ident: Quantum Radio. Generated commentary on the latest quantum physics and condensed matter papers.
Kai: I'm Kai.
Mira: And I'm Mira, here with Lev.
Kai: We're looking at the paper: "Controlled dewetting and phase transition hysteresis of VO2 nanostructures".
Mira: Here's the gist of the paper. Controlled dewetting and phase transition hysteresis of VO2 nanostructures demonstrates control over the phase transitions of VO2 nanocylinders via lithographic patterning, controlled crystallization, and controlled dewetting Because nanostructures are easier to address and consume less power than films, the ability to fabricate them with tailored geometry and hysteresis properties directly on integrated platforms is a key step toward scalable, energy-efficient memory and neuromorphic photonic devices.
Kai: Vanadium dioxide (VO2) exhibits an ultrafast, near-roomtemperature phase transition, characterized by hysteresis and large optical modulation—making it a promising candidate for short-term memories and for mimicking neural behavior in brainlike computing systems.
Mira: The VO2 phase transition exhibits hysteresis behavior, meaning the metal-insulator transition (MIT) occurs at lower temperatures than IMT, around 60 °C for bulk VO2.
Kai: While insufficient for long-term memories, as energy must be constantly supplied to store the information in the metallic phase, it is a good candidate for short-term memories and brain-like artificial neurons.
Title and authors: Kai: Let's talk about how they set up this study. The paper, "Controlled dewetting and phase transition hysteresis of VO2 nanostructures," focuses on using lithographic patterning and controlled crystallization to manage the phase transitions of VO2 nanocylinders.
Mira: The authors are looking at how different annealing temperatures affect these structures, because they know that temperature is a big lever for changing the morphology and the resulting phase change behavior.
Lev: I’m interested in what they actually built and measured. Are we talking about fabricated samples on a wafer, or just theoretical simulations? How realistic is this fabrication process for real hardware?
Kai: They fabricated six samples of amorphous VO2 nanocylinders with diameters ranging from one hundred twenty to nine hundred nanometers and annealed each one at different temperatures to see how the morphology changes.
Mira: That’s key because they found a deterministic dewetting window at seven hundred degrees Celsius where nanocylinders up to four hundred nanometers collapse into a single nanoparticle that saturates around two hundred twenty nanometers in size.
Lev: So, that gives us a specific target for how big we need our structures to be if we want them to behave predictably.
The paper's summary: Kai: What they’re summarizing is the correlation between the size of these nanostructures and their transition temperatures, hysteresis width, and optical modulation depth at one thousand five hundred nanometers wavelength.
Mira: They show that in grainy but continuous films annealed between five hundred and six hundred degrees Celsius, larger grains with fewer defects lead to broader hysteresis behavior.
Lev: That makes sense if you think about grain boundaries—they can create energy barriers that prolong the transition time or change where it happens. Does the paper confirm those grain boundaries are a primary driver of that broadening?
Kai: Yes, they do, and then they show that after the film dewets into separate nanoparticles, its hysteresis keeps broadening as those grain boundaries and defects almost disappear.
Mira: And then there's this part where they look at the regime between six hundred and seven hundred five hundred degrees Celsius where the nanoparticles are separated. They find that as these particles get smaller, the hysteresis further broadens because there are fewer nucleation centers to start with.
The paper's improvements: Kai: The authors suggest a few key improvements for how we approach this research. One big thing is tailoring memory properties by controlling the size of those nanostructures and annealing conditions to create a library of VO2 nanocylinders with desired hysteresis parameters.
Mira: They also point toward designing integrated platforms where these tailored geometry and hysteresis properties can be fabricated directly on integrated platforms, which is a major goal for scalable devices.
Lev: That’s the real engineering challenge, isn't it? Moving from a lab sample to something you can reliably put onto a chip where you control the environment around it.
Kai: And they suggest implementing deterministic dewetting windows at specific annealing temperatures so we can reliably control the number of resulting nanoparticles, which is crucial for encoding information into those structures.
Mira: They also look at optimizing particle size selection by leveraging light scattering resonance effects, like LSPR, to achieve a relatively high per-particle delta T while still maintaining a reasonably broad hysteresis.
Conclusion: Kai: So, to wrap up this study on "Controlled dewetting and phase transition hysteresis of VO2 nanostructures," the main implication is that we can now control the position, crystallization state, dewetting outcome, and the phase transition metrics of these structures with high precision.
Mira: This means we can select these nanostructures based on specific figure-of-merit metrics like transition temperatures and hysteresis widths, which are crucial for future compact neuromorphic photonic architectures.
Lev: From an error correction viewpoint, this level of control over the geometry and phase transition dynamics could potentially reduce the overhead you need to manage when running these systems on real hardware.
Kai: Exactly. We can finally decide whether we want maximum hysteresis width for stability or more optical contrast for modulation depth, because they often pull in opposite directions for a given volume of VO2.
Mira: It’s a trade-off that designers have to make when choosing the right material platform for their specific application.
Lev: So, controlling the phase transition at this nanoscale gives us a much better handle on the switching dynamics than we had before when dealing with bulk materials or films alone.
Kai: That's what this paper demonstrates about controlling dewetting and phase transition hysteresis of VO2 nanostructures.
Peter Kepćic, Petra Kalouskovľ Kalouskovľ, Tomľash Ŧikola, Filip Ligmajer
Brno University of Technology · Central European Institute of Technology
cond-mat.mes-hall, cond-mat.mtrl-sci, physics.optics
Submitted: 2026-04-07
Updated: 2026-04-07
Journal ref: ACS Appl. Nano Mater. (2026) 9 (27) 13013-13019
License: http://creativecommons.org/licenses/by/4.0/
Importance score: 78/100
The gist: Controlled dewetting and phase transition hysteresis of VO2 nanostructures demonstrates control over the phase transitions of VO2 nanocylinders via lithographic patterning…
Key concepts
- VO2 Phase Transition
- Vanadium dioxide (VO2) undergoes a rapid metal-insulator transition near room temperature. This transition exhibits hysteresis, meaning the switch between metallic and insulating states depends on the path taken (heating or cooling), which is key for memory applications.
- Dewetting
- Dewetting is the process where thin VO2 films separate into individual nanoparticles (NPs) during annealing. The thickness of the initial film determines whether this occurs, requiring higher temperatures for thicker films, and this morphology significantly affects the resulting phase transition properties.
- Hysteresis Width
- Hysteresis width refers to the range of temperatures over which a material can switch between its metallic and insulating states. Controlling this width allows designers to tailor memory stability; a broader hysteresis means more robust retention, while narrower hysteresis changes the switching characteristics.
Terminology
Summary
Controlled dewetting and phase transition hysteresis of VO2 nanostructures demonstrates control over the phase transitions of VO2 nanocylinders via lithographic patterning, controlled crystallization, and controlled dewetting Because nanostructures are easier to address and consume less power than films, the ability to fabricate them with tailored geometry and hysteresis properties directly on integrated platforms is a key step toward scalable, energy-efficient memory and neuromorphic photonic devices. p. 0 Here, we demonstrate control over the phase transitions of VO2 nanocylinders via lithographic
patterning, controlled crystallization, and controlled dewetting. Because nanostructures are
easier to address and consume less power than films, the ability to fabricate them with tailored
geometry and hysteresis properties directly on integrated platforms is a key step toward scalable,
energy-efficient memory and neuromorphic photonic devices. Here, we demonstrate control over the phase transitions of VO2 nanocylinders via lithographic
patterning, controlled crystallization, and controlled dewetting. Because nanostructures are
easier to address and consume less power than films, the ability to fabricate them with tailored
geometry and hysteresis properties directly on integrated platforms is a key step toward scalable,
energy-efficient memory and neuromorphic photonic devices.Where the paper says it
Where the paper says it
Introduction to VO2 Phase Transition Materials
Vanadium dioxide (VO2) exhibits an ultrafast, near-roomtemperature phase transition, characterized by hysteresis and large optical modulation—making it a promising candidate for short-term memories and for mimicking neural behavior in brainlike computing systems. The VO2 phase transition exhibits hysteresis behavior, meaning the metal-insulator transition (MIT) occurs at lower temperatures than IMT, around 60 °C for bulk VO2. p. 1 4,5 Such a low transition
temperature facilitates fabrication of memory devices made of microscale VO2 films that require
only picojoules of energy to switch. 6,7 Besides the ultrafast and low-energy transition, the VO2
phase transition exhibits hysteresis behavior, meaning the metal-insulator transition (MIT) occurs
at lower temperatures than IMT, around 60 ◦C for bulk VO2. 6,7 Besides the ultrafast and low-energy transition, the VO2
phase transition exhibits hysteresis behavior, meaning the metal-insulator transition (MIT) occurs
at lower temperatures than IMT, around 60 ◦C for bulk VO2. While insufficient for long-term
memories, as energy must be constantly supplied to store the information in the metallic phase, it
is a good candidate for short-term memories and brain-like artificial neurons. 8,9 In such devices,
the information can be written by a switching pulse and read by low-power pulses that follow
within the 101–102 ns window after. 10,11 To reduce the switching or retention energy and prolong
the retention time, the MIT and overall hysteresis characteristics can be tailored by adjusting stoichiometry, strain, volume, defects, and doping.Where the paper says it
Where the paper says it
Where the paper says it
Effect of Annealing on Film Morphology
The effect of annealing temperature on VO2 films is demonstrated by examining morphological changes after annealing under oxygen flow. The process of thin-film dewetting into separate NPs is strongly dependent on the initial film thickness, with thicker films requiring higher annealing temperatures and times, or even rendering dewetting practically impossible. p. 3 14,28 Note that
a similar behavior was also reported recently for continuous films annealed at prolonged times. 14
The process of thin-film dewetting into separate NPs is strongly dependent on the initial film
thickness, with thicker films requiring higher annealing temperatures and times, or even rendering
dewetting practically impossible. 14,28 Note that
a similar behavior was also reported recently for continuous films annealed at prolonged times. 14
The process of thin-film dewetting into separate NPs is strongly dependent on the initial film
thickness, with thicker films requiring higher annealing temperatures and times, or even rendering
dewetting practically impossible. 14
The process of thin-film dewetting into separate NPs is strongly dependent on the initial film
thickness, with thicker films requiring higher annealing temperatures and times, or even rendering
dewetting practically impossible. 14 The increasing annealing temperature leads not only to these
morphological changes, but also to an increase in IMT temperature and to a decrease in MIT
4Where the paper says it
Where the paper says it
Where the paper says it
-
At 500 °C, the VO2 grains become coarser (from 1 nm to 14 nm RMS roughness). p. 3
p. 3Where the paper says it
As the films were deposited onto amorphous fused silica substrates and annealed ex situ (post-deposition), they exhibited a polycrystalline character (Figure S1). Figure 1b shows that by increasing the annealing temperature above 500 ◦C, the VO2 grains become coarser (from 1 nm to 14 nm RMS roughness).
Where the paper says it
As the films were deposited onto amorphous fused silica substrates and annealed ex situ (post-deposition), they exhibited a polycrystalline character (Figure S1). Figure 1b shows that by increasing the annealing temperature above 500 ◦C, the VO2 grains become coarser (from 1 nm to 14 nm RMS roughness).
-
Above 600 °C, the films dewet into individual VO2 NPs, which then further aggregate. p. 3
p. 3Where the paper says it
Figure 1b shows that by increasing the annealing temperature above 500 ◦C, the VO2 grains become coarser (from 1 nm to 14 nm RMS roughness). Moreover, above 600 ◦C, the films dewet into individual VO2 NPs, which then further aggregate.
Where the paper says it
Figure 1b shows that by increasing the annealing temperature above 500 ◦C, the VO2 grains become coarser (from 1 nm to 14 nm RMS roughness). Moreover, above 600 ◦C, the films dewet into individual VO2 NPs, which then further aggregate.
-
At 750 °C, these NPs begin to wet (spread) and seemingly shrink due to oxidation toward the more volatile V2O5 stoichiometry. p. 3
p. 3Where the paper says it
Moreover, above 600 ◦C, the films dewet into individual VO2 NPs, which then further aggregate. Finally, at 750 ◦C, these NPs begin to wet (spread) and seemingly shrink due to oxidation toward the more volatile V2O5 stoichiometry, which exhibits a lower contact angle and forms a “skirt” around the nanoparticle.
Where the paper says it
Moreover, above 600 ◦C, the films dewet into individual VO2 NPs, which then further aggregate. Finally, at 750 ◦C, these NPs begin to wet (spread) and seemingly shrink due to oxidation toward the more volatile V2O5 stoichiometry, which exhibits a lower contact angle and forms a “skirt” around the nanoparticle.
Size-Dependent Hysteresis and Optical Modulation
The study correlates nanostructure size and annealing conditions with transition temperatures, hysteresis width, and optical modulation.
-
In grainy but continuous films (500–650 °C), large grains with fewer defects result in broader hysteresis. p. 4
p. 4Where the paper says it
Thus, although hysteresis continues to broaden with smaller NPs, the optical contrast diminishes. This dependence of hysteresis widths and ΔT1550 nm confirms two physical effects related to regimes of grainy films and separated NPs:14 In grainy but continuous films (500–650 ◦C), large grains with fewer defects result in broader hysteresis, as there are fewer oxygen vacancies at grain boundaries to initiate the nucleation of one phase in another.
Where the paper says it
Thus, although hysteresis continues to broaden with smaller NPs, the optical contrast diminishes. This dependence of hysteresis widths and ΔT1550 nm confirms two physical effects related to regimes of grainy films and separated NPs:14 In grainy but continuous films (500–650 ◦C), large grains with fewer defects result in broader hysteresis, as there are fewer oxygen vacancies at grain boundaries to initiate the nucleation of one phase in another.
-
After the film dewets into separated NPs, its hysteresis continues to broaden as the grain boundaries and defects almost disappear. p. 4
p. 4Where the paper says it
This dependence of hysteresis widths and ΔT1550 nm confirms two physical effects related to regimes of grainy films and separated NPs:14 In grainy but continuous films (500–650 ◦C), large grains with fewer defects result in broader hysteresis, as there are fewer oxygen vacancies at grain boundaries to initiate the nucleation of one phase in another. 17 After the film dewets into separated NPs, its hysteresis continues to broaden as the grain boundaries and defects almost disappear.
Where the paper says it
This dependence of hysteresis widths and ΔT1550 nm confirms two physical effects related to regimes of grainy films and separated NPs:14 In grainy but continuous films (500–650 ◦C), large grains with fewer defects result in broader hysteresis, as there are fewer oxygen vacancies at grain boundaries to initiate the nucleation of one phase in another. 17 After the film dewets into separated NPs, its hysteresis continues to broaden as the grain boundaries and defects almost disappear.
-
In the regime of separated NPs (between 650–750 °C), as the NPs get smaller, the hysteresis further broadens, as the amount of nucleation centers decreases with the decreasing size. p. 5
p. 5Where the paper says it
In the regime of separated NPs (between 650–750 ◦C), as the NPs get smaller (see Figure S1), the hysteresis further broadens, as the amount of nucleation centers decreases with the decreasing size. 18,20,21 The path towards hysteresis broadening is thus two-fold: smaller isolated NPs or larger grains within the polycrystalline film.
Where the paper says it
In the regime of separated NPs (between 650–750 ◦C), as the NPs get smaller (see Figure S1), the hysteresis further broadens, as the amount of nucleation centers decreases with the decreasing size. 18,20,21 The path towards hysteresis broadening is thus two-fold: smaller isolated NPs or larger grains within the polycrystalline film.
-
While grain growth within VO2 films at medium annealing temperatures increases ΔT1550 nm, the subsequent dewetting and shrinking of separated NPs at larger annealing temperatures decrease it. p. 5
p. 5Where the paper says it
18,20,21 The path towards hysteresis broadening is thus two-fold: smaller isolated NPs or larger grains within the polycrystalline film. However, in the context of optical modulation, these two strategies lead to opposite results: While the grain growth within VO2 films at medium annealing temperatures increases ΔT1550 nm, the subsequent dewetting and shrinking of separated NPs at larger annealing temperatures decrease it.
Where the paper says it
18,20,21 The path towards hysteresis broadening is thus two-fold: smaller isolated NPs or larger grains within the polycrystalline film. However, in the context of optical modulation, these two strategies lead to opposite results: While the grain growth within VO2 films at medium annealing temperatures increases ΔT1550 nm, the subsequent dewetting and shrinking of separated NPs at larger annealing temperatures decrease it.
Control Over Nanocylinder Dewetting
The authors fabricated six samples of amorphous VO2 nanocylinders with diameters ranging from 120 to 900 nm and annealed each at different temperatures. The morphological changes of nanocylinders after annealing are analogous to those of the films. p. 7 Similar behavior, but shifted to smaller measured diameters, can be observed for NPs obtained
after dewetting the nanocylinders at even higher temperature of 750 ◦C (see Figure S2). These
results indicate that the morphological changes of nanocylinders after annealing are analogous to
those of the films: Until the annealing temperature is high enough to cause dewetting into NPs,
the diameters of nanocylinders after annealing are unaffected, while their heights/volumes grow
8Where the paper says it
-
The process shows that until the annealing temperature is high enough to cause dewetting into NPs, the diameters of nanocylinders after annealing are unaffected, while their heights/volumes grow significantly. p. 7
Where the paper says it
Similar behavior, but shifted to smaller measured diameters, can be observed for NPs obtained after dewetting the nanocylinders at even higher temperature of 750 ◦C (see Figure S2). These results indicate that the morphological changes of nanocylinders after annealing are analogous to those of the films: Until the annealing temperature is high enough to cause dewetting into NPs, the diameters of nanocylinders after annealing are unaffected, while their heights/volumes grow 8
-
A deterministic dewetting window at 700 °C was identified: nanocylinders with diameters up to 400 nm predominantly collapse into a single NP, whose diameter saturates near 220 nm, whereas larger nanocylinders dewet stochastically into multiple particles. p. 7
Where the paper says it
The diameters of dewetted NPs are approximately 60 % of the initial nanocylinders, up to the diameter of 400 nm. Beyond this threshold, their average diameter asymptotically approaches 220 nm, while their variance increases significantly due to dewetting of these larger nanocylinders into more than one NP (see below).
Tuning Hysteresis and Optical Contrast
Optical hysteresis measurements at 1550 nm reveal a robust, size-dependent tuning of hysteresis width that decays exponentially with the increasing nanocylinder diameter (with convergence to film-like behavior above 400 nm).
-
The hysteresis width decreases from 56 °C at 120 nm diameter to 50 °C at 400 nm diameter, and ultimately to 48 °C, when nanocylinders dewet into multiple NPs. p. 7
Where the paper says it
Around them, a very thin (5±5)nm non-uniform polycrystalline residue remains in the original footprint of the cylinder (essentially a faint ’shadow’ of the former nanocylinder, see Figure 2a). The diameters of dewetted NPs are approximately 60 % of the initial nanocylinders, up to the diameter of 400 nm.
-
The transmittance modulation follows the same annealing trends as films and can be significantly enhanced by LSPR for 400–600 nm diameters. p. 5
Where the paper says it
However, in the context of optical modulation, these two strategies lead to opposite results: While the grain growth within VO2 films at medium annealing temperatures increases ΔT1550 nm, the subsequent dewetting and shrinking of separated NPs at larger annealing temperatures decrease it. As the NPs get smaller, the overall transmittance in both VO2 phases increases due to their smaller surface coverage.
-
Designers must decide between maximizing hysteresis width (memory-state stability) and optical contrast, as these are opposing effects for a given VO2 volume. p. 4
Where the paper says it
Thus, although hysteresis continues to broaden with smaller NPs, the optical contrast diminishes. This dependence of hysteresis widths and ΔT1550 nm confirms two physical effects related to regimes of grainy films and separated NPs:14 In grainy but continuous films (500–650 ◦C), large grains with fewer defects result in broader hysteresis, as there are fewer oxygen vacancies at grain boundaries to initiate the nucleation of one phase in another.
Conclusion on Device Potential
Collectively, these results demonstrate scalable control over position, crystallization state, dewetting outcome, and phase-transition metrics. These nanostructures can then be selected based on specific figure-of-merit metrics (transition temperatures, hysteresis widths, modulation depths), which are crucial for future compact, energy-efficient, tunable, and neuromorphic photonic architectures. p. 2 Such a library is essential for the design and fabrication of energy-efficient VO2
nanostructures for multilevel memory and neuromorphic photonic devices. Results and discussion
Phase transition hysteresis of VO2 films. As the VO2 transforms into smaller isolated NPs, the overall transmission increases and
ΔT1550 nm decreases, since NPs cover less surface and in the metallic phase support a localized
surface plasmon resonance (LSPR) that shifts out of the 1550 nm wavelength as size decreases
(discussed in more detail later in the text). Thus, although hysteresis continues to broaden with
smaller NPs, the optical contrast diminishes.Where the paper says it
Where the paper says it
Acknowledgement
This work is supported by the Grant Agency of the Czech Republic (project No. 25-18336M) and by the Ministry of Education, Youth and Sports of the Czech Republic (project No. p. 0 Controlled dewetting and phase transition
hysteresis of VO2 nanostructures
Peter Kepič,† Petra Kalousková,‡ Tomáš Šikola,†,‡ and Filip Ligmajer∗,†,‡
†Brno University of Technology, Central European Institute of Technology, Purkyňova 123,
612 00, Brno, Czech Republic
‡Brno University of Technology, Faculty of Mechanical Engineering, Technická 2,
616 69, Brno, Czech Republic
E-mail: filip. ligmajer@ceitec. b) Hysteresis
width and c) ΔT1550 nm of VO2 nanocylinders annealed at 500 ◦C, 600 ◦C, and 700 ◦C as functions of
the designed nanocylinder diameter. Note that absolute ΔT values for nanocylinders appear lower
than for films in Figure 1 due to different measurement setups and fill-factors, so comparisons
should be just qualitative.Where the paper says it
Where the paper says it
References
-
Lian, C.; Vagionas, C.; Alexoudi, T.; Pleros, N.; Youngblood, N.; Ríos, C. Photonic (computational) memories: tunable nanophotonics for data storage and computing
-
Lopez, R.; Haglund, R. F.; Feldman, L. C.; Boatner, L. A.; Haynes, T. E. Optical nonlinearities in VO2 nanoparticles and thin films
-
O’Callahan, B. T.; Jones, A. C.; Park, J. H.; Cobden, D. H.; Atkin, J. M.; Raschke, M. B. Inhomogeneity of the ultrafast insulator-to-metal transition dynamics of VO2
-
Morin, F. J. Oxides Which Show a Metal-to-Insulator Transition at the Neel Temperature
-
Kepič, P.; Ligmajer, F. p. 0
p. 0Where the paper says it
Controlled dewetting and phase transition hysteresis of VO2 nanostructures Peter Kepič,† Petra Kalousková,‡ Tomáš Šikola,†,‡ and Filip Ligmajer∗,†,‡ †Brno University of Technology, Central European Institute of Technology, Purkyňova 123, 612 00, Brno, Czech Republic ‡Brno University of Technology, Faculty of Mechanical Engineering, Technická 2, 616 69, Brno, Czech Republic E-mail: filip. ligmajer@ceitec.
; Hrtoň, M.; Ren, H.; de S. Menezes, L.; Maier, S. A.; Šikola, T. p. 0Where the paper says it
Controlled dewetting and phase transition hysteresis of VO2 nanostructures Peter Kepič,† Petra Kalousková,‡ Tomáš Šikola,†,‡ and Filip Ligmajer∗,†,‡ †Brno University of Technology, Central European Institute of Technology, Purkyňova 123, 612 00, Brno, Czech Republic ‡Brno University of Technology, Faculty of Mechanical Engineering, Technická 2, 616 69, Brno, Czech Republic E-mail: filip. ligmajer@ceitec.
p. 0Where the paper says it
Controlled dewetting and phase transition hysteresis of VO2 nanostructures Peter Kepič,† Petra Kalousková,‡ Tomáš Šikola,†,‡ and Filip Ligmajer∗,†,‡ †Brno University of Technology, Central European Institute of Technology, Purkyňova 123, 612 00, Brno, Czech Republic ‡Brno University of Technology, Faculty of Mechanical Engineering, Technická 2, 616 69, Brno, Czech Republic E-mail: filip. ligmajer@ceitec.
Optically Tunable Mie Resonance VO2 Nanoantennas for Metasurfaces in the VisibleWhere the paper says it
Controlled dewetting and phase transition hysteresis of VO2 nanostructures Peter Kepič,† Petra Kalousková,‡ Tomáš Šikola,†,‡ and Filip Ligmajer∗,†,‡ †Brno University of Technology, Central European Institute of Technology, Purkyňova 123, 612 00, Brno, Czech Republic ‡Brno University of Technology, Faculty of Mechanical Engineering, Technická 2, 616 69, Brno, Czech Republic E-mail: filip. ligmajer@ceitec.
-
Jung, Y.; Han, H.; Sharma, A.; Jeong, J.; Parkin, S. S. P.; Poon, J. K. S. Integrated Hybrid VO2–Silicon Optical Memory
-
Parra, J.; Navarro-Arenas, J.; Sanchis, P. Sub-milliwatt Threshold Power and Tunable-Bias All-Optical Nonlinear Activation Function Using Vanadium Dioxide for Wavelength-Division Multiplexing Photonic Neural Networks
-
Schofield, P.; Bradicich, A.; Gurrola, R. M.; Zhang, Y.; Brown, T. D.; Pharr, M.; Shamberger, P. J.; Banerjee, S. Harnessing the Metal–Insulator Transition of VO2 in Neuromorphic Computing
-
Lee, Y. J.; Kim, Y.; Gim, H.; Hong, K.; Jang, H. W. Nanoelectronics Using Metal–Insulator Transition
-
Rini, M.; Cavalleri, A.; Schoenlein, R. W.; López, R.; Feldman, L. C.; Haglund, R. F.; Boatner, L. A.; Haynes, T. E. Photoinduced Phase Transition in VO2 Nanocrystals: Ultrafast Control of Surface-Plasmon Resonance
-
Ryckman, J. D.; Hallman, K. A.; Marvel, R. E.; Haglund, R. F.; Weiss, S. M. Ultra-Compact Silicon Photonic Devices Reconfigured by an Optically Induced Semiconductor-to-Metal Transition
-
Andrews, J. L.; Santos, D. A.; Meyyappan, M.; Williams, R. S.; Banerjee, S. Building BrainInspired Logic Circuits from Dynamically Switchable Transition-Metal Oxides
-
Kaufman, M.; Vlček, J.; Houška, J.; Farrukh, S.; Haviar, S. Design and Scalable Synthesis of Thermochromic VO2-Based Coatings for Energy-Saving Smart Windows with Exceptional Optical Performance
-
White, S. T.; Taylor, J. R.; Chukhryaev, I.; Bailey, S. M.; Queen, J. M.; McBride, J. R.; Haglund, R. F. Solid-State Dewetting of Tungsten-Doped Vanadium Dioxide Nanoparticles: Implications for Thermochromic Coatings
-
Breckenfeld, E.; Kim, H.; Burgess, K.; Charipar, N.; Cheng, S.-F.; Stroud, R.; Piqué, A. Strain Effects in Epitaxial VO2 Thin Films on Columnar Buffer-Layer TiO2/Al2O3 Virtual Substrates
-
White, S. T.; Thompson, E. A.; Brown, P. F.; Haglund, R. F. Substrate Chemistry and Lattice Effects in Vapor Transport Growth of Vanadium Dioxide Microcrystals
-
Appavoo, K.; Lei, D. Y.; Sonnefraud, Y.; Wang, B.; Pantelides, S. T.; Maier, S. A.; Haglund, R. F. Role of Defects in the Phase Transition of VO2 Nanoparticles Probed by Plasmon Resonance Spectroscopy
-
Lopez, R.; Haynes, T. E.; Boatner, L. A.; Feldman, L. C.; Haglund, R. F. Size effects in the structural phase transition of VO2 nanoparticles
-
Donev, E. U.; Lopez, R.; Feldman, L. C.; Haglund, R. F. Confocal Raman Microscopy Across The Metal-Insulator Transition of Single Vanadium Dioxide Nanoparticles
-
Clarke, H.; Carraway, B. D.; Sellers, D. G.; Braham, E. J.; Banerjee, S.; Arróyave, R.; Shamberger, P. J. Nucleation-controlled hysteresis in unstrained hydrothermal VO2 particles
16 (Note: Reference 16 appears twice in the provided text list for different contexts)
-
Nishikawa, K.; Nishida, J.; Yoshimura, M.; Nakamoto, K.; Kumagai, T.; Watanabe, Y. Metastability in the Insulator–Metal Transition for Individual Vanadium Dioxide Nanoparticles
-
Kepič, P.; Horák, M.; Kabát, J.; Hájek, M.; Konečná, A.; Šikola, T.; Ligmajer, F. Coexisting Phases of Individual VO2 Nanoparticles for Multilevel Nanoscale Memory
-
Griffiths, C. H.; Eastwood, H. K. Influence of Stoichiometry on the Metal–Semiconductor Transition in Vanadium Dioxide
-
Shvets, P.; Dikaya, O.; Maksimova, K.; Goikhman, A. A Review of Raman Spectroscopy of Vanadium Oxides
-
Rampelberg, G.; De Schutter, B.; Devulder, W.; Martens, K.; Radu, I.; Detavernier, C. In Situ X-ray Diffraction Study of the Controlled Oxidation and Reduction in the V–O System for the Synthesis of VO2 and V2O3 Thin Films
-
Shibuya, K.; Sawa, A. Optimization of Conditions for Growth of Vanadium Dioxide Thin Films on Silicon by Pulsed-Laser Deposition
-
Marvel, R. E.; Harl, R. R.; Craciun, V.; Rogers, B. R.; Haglund, R. F. Influence of Deposition Process and Substrate on the Phase Transition of Vanadium Dioxide Thin Films
-
Suh, J. Y.; Lopez, R.; Feldman, L. C.; Haglund, R. F. Semiconductor to Metal Phase Transition in the Nucleation and Growth of VO2 Nanoparticles and Thin Films
-
Alcaide, A. M.; Regodon, G.; Ferrer, F. J.; Rico, V.; Alvarez, R.; Rojas, T. C.; González
-
Wen, H.; Guo, L.; Barnes, E.; Lee, J. H.; Walko, D. A.; Schaller, R. D.; Moyer, J. A.; Misra, R.; Li, Y.; Dufresne, E. M.; Schlom, D. G.'; Gopalan, V.'; Freeland, J. W.'; Structural and Electronic Recovery Pathways of a Photoexcited Ultrathin VO2 Film
-
Wu, L.; Fu, H.; Li, S.; Zhu, J.; Zhou, J.; Rao, A. M.; Cha, L.; Guo, K.; Wen, S.'; Lu, B. PhaseEngineered Cathode for Super-Stable Potassium Storage
-
Li, J.; Navarro; Pofelski, A.; Salev, P.; El Hage, R.; Qiu, E.; Zhu, Y.; Fainman, Y.; Schuller, I. Laser-Induced Selective Local Patterning of Vanadium Oxide Phases
18 (Note: Reference 18 appears twice in the provided text list for different contexts)
19 (Note: Reference 19 appears twice in the provided text list for different contexts)
20 (Note: Reference 20 appears twice in the provided text list for different contexts)
(Self-Correction Note: The final output must strictly adhere to the requested format, including token placement and anchoring.)
Pruning redundant reasoning tokens
The paper demonstrates control over the phase transitions of VO2 nanocylinders via lithographic patterning, controlled crystallization, and controlled dewetting. Because nanostructures are easier to address and consume less power than films, the ability to fabricate them with tailored geometry and hysteresis properties directly on integrated platforms is a key step toward scalable, energy-efficient memory and neuromorphic photonic devices.
How the training signal is built
The effect of annealing temperature on VO2 films is demonstrated by examining morphological changes after annealing under oxygen flow. The process of thin-film dewetting into separate NPs is strongly dependent on the initial film thickness, with thicker films requiring higher annealing temperatures and times, or even rendering dewetting practically impossible.
-
At 500 °C, the VO2 grains become coarser (from 1 nm to 14 nm RMS roughness).
-
Above 600 °C, the films dewet into individual VO2 NPs, which then further aggregate.
-
At 750 °C, these NPs begin to wet (spread) and seemingly shrink due to oxidation toward the more volatile V2O5 stoichiometry.
Where the gains come from
The study correlates nanostructure size and annealing conditions with transition temperatures, hysteresis width, and optical modulation.
-
In grainy but continuous films (500–650 °C), large grains with fewer defects result in broader hysteresis.
-
After the film dewets into separated NPs, its hysteresis continues to broaden as the grain boundaries and defects almost disappear.
-
In the regime of separated NPs (between 650–750 °C), as the NPs get smaller, the hysteresis further broadens, as the amount of nucleation centers decreases with the decreasing size.
-
While grain growth within VO2 films at medium annealing temperatures increases ΔT1550 nm, the subsequent dewetting and shrinking of separated NPs at larger annealing temperatures decrease it.
Green — the paper says it, and the page is printed. Red — no passage carries it, so treat that sentence as unverified. The same check runs on your own text: check a summary against its source, $5.
Improvements for AI systems
-
Tailor memory properties by controlling nanostructure size and annealing conditions to create a library of VO2 nanocylinders with desired hysteresis parameters for multilevel memory and neuromorphic photonic devices.
-
Design integrated platforms where tailored geometry and hysteresis properties of VO2 nanostructures can be fabricated directly on integrated platforms, leading toward scalable, energy-efficient memory and neuromorphic photonic devices.
-
Implement deterministic dewetting windows at specific annealing temperatures to reliably control the number of resulting nanoparticles, which is crucial for encoding information into the size of nanostructures.
-
Optimize particle size selection by leveraging LSPR effects to achieve a relatively high per-particle Delta T while still maintaining a reasonably broad hysteresis, allowing designers to choose between maximizing hysteresis width and optical contrast.
Abstract
As artificial intelligence continues to grow, so does the need for more efficient ways to process data. Besides moving from electronic to photonic circuits, a promising approach is to integrate phase-change materials. Vanadium dioxide (VO 2) exhibits an ultrafast, near-room-temperature phase transition, characterized by hysteresis and large optical modulation -- making it a promising candidate for short-term memories and for mimicking neural behavior in brain-like computing systems. While the hysteresis behavior of VO 2 has been well studied in thin films and nanostructures, practical control and device integration have been limited only to thin films. Here, we demonstrate control over the phase transitions of VO 2 nanocylinders via lithographic patterning, controlled crystallization, and controlled dewetting. Because nanostructures are easier to address and consume less power than films, the ability to fabricate them with tailored geometry and hysteresis properties directly on integrated platforms is a key step toward scalable, energy-efficient memory and neuromorphic photonic devices.
Related papers
- Coexistence of polariton bound states in the continuum and 2D radiative excitons
- Hidden Quantum-Geometric Connection between Injection and Shift Currents
- Specific absorption rate of uniaxial single-domain nanomagnets: stochastic spin dynamics versus linear response theory
- The ideal limit of rhombohedral graphene: Dynamical skyrmion lattices and their excitations
- Valley polarization of chiral excitonic bound states induced by band geometry
- On-Device Control of Electronic Friction